Table 2.7.3| top | pdf |
Parameters recommended for pressure determination by EOS measurements

Various face-centred cubic (f.c.c.) and body-centred cubic (b.c.c.) metals are used as calibrants, with the EOS given by equation (2.7.1)[link] and the reference temperature TR = 300 K (after Holzapfel, 1997[link]).

Metala0R (pm)K0R (GPa)K0Rα0R (× 106 K)δαR
Al 404.98 (1) 72.5 (4) 4.8 (2) 23.0 (4) 5.5 (11)
Cu 361.55 (1) 133.2 (2) 5.4 (2) 16.6 (3) 6.1 (6)
Ag 408.62 (1) 101.0 (2) 6.2 (2) 19.2 (4) 7.1 (6)
Au 407.84 (1) 166.7 (2) 6.3 (2) 14.2 (2) 7.2 (6)
Pd 388.99 (1) 189 (3) 5.3 (2) 11.6 (4) 6.0 (11)
Pt 392.32 (1) 277 (5) 5.2 (2) 8.9 (4) 5.9 (l1)
Mo 314.73 (1) 261 (5) 4.5 (5) 5.0 (4) 5.2 (14)
W 316.47 (1) 308 (2) 4.0 (2) 4.5 (4) 4.7 (11)